• English
  • United States(USD $)
/ /

Coating product material 4.2

Aug 14,2022 | FOSHAN CAILONG METALLIC PACKAGING MATERIAL CO.,LTD

Metallized Product Material

High Barrier Metallized Film VMPET-GZ

Imported Equipment Metallized Film

Domestic Equipment Metallized Film

Al Thickness

Å

500~800

Al Thickness

Å

450~640

Al Adhesion

N/15mm

2.4~3.1

Al Adhesion 

N/15mm

1.5~3.0

OTR

cm³/(m²*24h*0.1Mpa),23℃

0.3~0.6

OTR

cm³/(m²*24h*0.1Mpa),23℃

0.6~0.7

WVTR

g/(m²*24h),100%,38℃

0.4~0.7

WVTR

g/(m²*24h),90%,38℃

0.35~0.8

 

 

Metallized Empty Lines VMPET

Imported Equipment Metallized Film

Domestic Equipment Metallized Film

Subtle or no metallized empty line

Obviously, at least one metallized empty line

 

 

Metallized Reflective Film VMPET

Imported Equipment Metallized Film

Domestic Equipment Metallized Film

Al Reflectance(%)

85~95

Al Reflectance(%)

85~90

 

 

Metallized Films OTR TEST

Imported Test Equipment

Domestic Test Equipment

OTR cm³/(m²*24h*0.1Mpa),23℃)

1.097

OTR cm³/(m²*24h*0.1Mpa),23℃)

1.390

 

 

Metallized Films WVTR TEST

Imported Test Equipment

Domestic Test Equipment

WVTR g/(m²*24h),100%,38℃

0.535

WVTR g/(m²*24h),90%,38℃

1.521

 

 

Al Adhesion Test

EAA Glue Peeling Method

Adhesive Tape Peeling Method

The EAA glue and the aluminum-plated surface are heat-sealed, using the peeling test to obtain the peeling force between the EAA glue and the aluminum-plated surface.

2.63 N/15mm

Paste the surface of the aluminum-plated layer with tape, peel off the tape, and

judge according to the drop-off area of the aluminum coating, the adhesion is difficult to quantify

S<10%